Why Hole Sizing Matters in Multi-Pass Moving Wire Coating
In continuous bottom-entry PTFE dispersion coating, each MWS must balance sealing contact against surface wear as coating thickness accumulates from pass to pass.
Hole too tight: PTFE “snow” and delayed leaks
Excessive radial squeeze presses the EPDM lip against coating from prior passes. On long runs, rubbing may generate microscopic PTFE debris (“snow”) that contaminates the bath or contributes to coating defects. High squeeze may also increase shear in dispersion at the seal throat and contribute to delayed weeping.
Hole too loose: dispersion weeping
Wetting surfactants lower the surface tension of aqueous PTFE dispersion. If circumferential contact is insufficient, liquid may pass the seal lip and reach the lower rollers. Dried residue can flake from the rollers and return to the bath with the wire.
Pass-by-pass wire growth
Each pass adds radial coating build, so the incoming wire OD increases at later seals. Evaluate each hole for the OD entering that pass. Roth Technologies’ initial recommendation is Medium Fit (5%) for bare wire on Pass 1 and Light Fit (2%) for later coated passes.
Starting fit reference — RT-MWS-TN-007 Rev R8: Light 2%, Medium 5%, and Heavy 8% interference. These are starting recommendations, not validated operating limits. End users should establish and verify fit guidance for their bath, fluid, line speed, wire, and equipment setup.
Read RT-MWS-TN-007 Rev R8: Hole-Sizing Theory & Multi-Pass Guidelines (PDF)Wire and seal inputs
Initial fit schedule: Pass 1 Medium (5%); later passes Light (2%). Change any pass independently. These percentages are model inputs for evaluation, not validated production recommendations.
Pass-by-pass results
Set wet friction coefficient μ separately for each pass. Each pass starts at 0.06; this is an editable estimate, not measured MWS data.
| Pass | Incoming OD (in) | Fit | Interference | Relaxed hole ID (in) | Wet μ | Normal force (gram-force) | Estimated drag (gram-force) |
|---|
Shop-Floor Hole Preparation & Inspection Guidelines (RT-MWS-TN-007, Rev R8)
- Target relaxed hole ID; do not assume punch recovery. The model does not apply a universal elastomer recovery percentage or predict punch OD. Recovery depends on the EPDM batch, punch sharpness, lubrication, backing, and technique; verify it by measuring trial seals after recovery.
- Punch outside-in on an internal support mandrel. Use a sharp hollow punch perpendicular to the seal tip against firm sacrificial backing. If a wetting agent is used, first confirm compatibility with the EPDM and process. Avoid needle punctures and rotating twist drills; inspect both cut faces.
- Inspect without stretching the hole. Use an optical comparator, toolmaker’s microscope, or calibrated vision system to check relaxed hole ID and inspect the cut edge. The R8 note recommends non-contact optical measurement rather than pin gauges or calipers for soft EPDM.
- Maintain alignment and control bath conditions. Align the lower guide roller with the MWS centerline to reduce lateral wire pull. Keep bath level as shallow as the process permits and consider drip protection during threading or line stops.
- Keep seals assigned to their pass. Mark housings P1, P2, and so on, and preserve each seal’s intended orientation.
View the complete R8 technical note (PDF)Model equations and scope
Hole diameter
Din,n = D0 + 2(n−1)(ttotal/N)Dh,n = Din,n(1−in)Normal force
FN = p · π · Dw · LThe finite-wall Lamé model calculates pressure internally; the page reports force in gram-force.
Wet sliding drag
Fdrag,n = μn · FN,nEach pass has an independently editable μ value.
This is a simplified linear-elastic, concentric-contact model with uniform pressure over the stated contact length. It does not model EPDM nonlinearity, lip deformation, adhesion, bath pressure, buildup, wear, or process performance. The page reports relaxed hole ID and does not apply an elastomer punch-recovery correction or predict punch OD/tooling size. Treat force and drag as engineering estimates and validate hole size, fit, and drag on the actual MWS, wire, and liquid.